Table 5. Tensile Properties of Post-Vulcanisable Loprol Examination Gloves

  LOPROL ASTM 3578-1991
A Unaged
Tensile strength (MPa)
Elongation at break (%)
M300 (MPa)
M500 (MPa)
 
25-27
850 - 900
1.15 - 1.25
2.00 - 2.12
 
>21
-700
-
-
B Aged (7 days/70°C)
Tensile strength (MPa)
Elongation at break
M300 (MPa)
M500 (MPa)
 
23 - 25
750 - 800
1.3 - 1.4
2.3 - 2.5
 
>16
-500
-
-
C Aged (1 day/100°C)
Tensile strength (MPa)
Elongation at break (%)
M300 (MPa) M500 (MPa)
 
23-27
790 - 830
1.2 -1.4
2.1 - 2.4
 
>16
-500
-
-